SUMMET METHOD FOR METAL MATRIX -COMPOSITES

Sectioning Precision Saw with 15HC blade recommended for metal matrix composites
Mounting Castable, typically epoxy
Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Apex DGD Yellow 35 µm diamond water cooled 5 [22] 300 Rotation Image Until Plane
UltraPad 9 µm MetaDi Supreme Diamond 5 [22] 150 Rotation Image 4:00
VerduTex 3 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 3:00
ChemoMet 0.02 -0.06 µm MasterMet or MasterMet 2 Colloidal Silica 6 [27] 150 Rotation Image 1:30